Academic Jobs - Home of Higher Ed Logo

Research spotlight: Tahmina Keya on what really decides cavitation erosion damage

8 min read12 views

At a glance

Tahmina Keya and colleagues tested aluminium, copper alloys and stainless steel in a cavitating jet and found that no single mechanical property predicts cavitation erosion rates.

a close up of a scrabble tile wall with words written on it
Photo by Monica Flores on Unsplash

Two metal coupons, one tank of water, one high-pressure jet. After identical exposure, the aluminium alloy has given up 171 times more material than the bronze. That ratio sits at the centre of a study in Tribology International that asks a question every pump and turbine designer eventually faces: which mechanical property tells you how a metal will behave when bubbles start collapsing on it?

The answer, from Tahmina Keya and five co-authors, is that none of them does on its own.

The team put AA 6063 aluminium, pure copper, bronze, a copper-nickel alloy and 316L stainless steel through a cavitating jet apparatus built to the ASTM G134 standard, then ran the same materials through microhardness, depth-sensing indentation, quasi-static and high-strain-rate tests. Spearman-style correlation hunting followed: which property moves in step with the erosion rate, and how tightly.

Why a metal's worst day matters to a power station

Cavitation is water boiling without heat. Drop the local pressure below the liquid's vapour pressure and it tears open into vapour pockets. A few centimetres downstream, where pressure recovers, those pockets collapse. Each collapse lasts microseconds and fires a microjet of water at the neighbouring wall at hundreds of metres per second, over and over, thousands of times a second.

On a Francis turbine runner, that is enough to pit a polished steel surface in hours and to chew craters into it over a few seasons. Weld repair restores the metal but changes the blade profile that was designed to tight tolerances, and the damaged zone often returns. So the choice of alloy at the design stage carries years of consequences: outage scheduling, spare-part logistics, the price of electricity from that unit.

Yet erosion resistance is rarely specified with the same rigour as yield strength. Procurement documents lean on hardness because hardness is on every datasheet and cheap to verify. Keya's results suggest that shortcut leaves real information on the table.

How to erode a metal on purpose

ASTM G134 describes how to damage a specimen reproducibly with a cavitating liquid jet. Water is forced through a nozzle into a chamber held at a controlled lower pressure, cavitation forms in the shear layer of the jet, and the resulting bubble clouds collapse against a stationary specimen held at a set stand-off distance.

Run that long enough and you get a cumulative erosion curve, which the standard reads as two numbers. The incubation period is the stretch where mass loss is negligible while the surface pits and work-hardens. The maximum erosion rate, or MER, is the steepest part of the curve, where material leaves as fast as it ever will. MER is what this study correlated against mechanical properties.

The mechanical side of the experiment is where the paper earns its title. Microhardness gives one number. Depth-sensing indentation adds plastic indentation work, the energy a surface soaks up while a hard tip presses a permanent dent into it, plus a wear resistance index derived from the same data. Quasi-static testing supplied ultimate strength and toughness. High-strain-rate testing supplied flow stress under loading fast enough to resemble a bubble collapse rather than a laboratory tensile machine pulling at millimetres per minute.

Text from a book with religious verses

Photo by Brett Jordan on Unsplash

What the correlations showed

Six properties tracked the damage, all in the same direction: more of the property, less erosion. As hardness increased, MER fell. Same for plastic indentation work. Same for the wear resistance index. Same again for toughness, ultimate strength and flow stress. Bronze, the most erosion-resistant material in the set, sat at the favourable end of those rankings; AA 6063 aluminium sat at the bottom, and by a wide margin.

The authors' summary is unhedged. Their results, they write, revealed that "cavitation erosion does not correlate with a single property."

Hardness and toughness get confused constantly, and this is a useful place to separate them. Hardness is how much pressure it takes to leave a dent. Toughness is how much work it takes to break something that has already started to yield. A ceramic floor tile is hard and not tough: a key won't scratch it, and a dropped mug will crack it. Bubble collapse is a denting problem and a breaking problem at once, repeated micro-impact that deforms a thin surface layer, cracks it, then tears flakes out of the cracked metal. An alloy that only resists the dent won't help you once the damage front starts to fracture.

That is why the strongest single correlations in the paper come from tests that push past the elastic limit, and why relying on hardness alone is like judging a boxer by his jaw and ignoring his ribs.

Where the evidence stops

Five alloys is a thin population for a correlational claim, and the paper does not pretend otherwise. One aluminium, three copper-based alloys and one stainless steel span a useful range of erosion behaviour. They don't support a general equation that predicts MER from a materials certificate.

Everything ran in one rig at one jet intensity in one liquid, water. That matters more than it sounds. Published work on ASTM G134 has found maximum cumulative erosion rates shifting by more than 600 percent across different nozzle geometries, which is precisely why the standard fixes a nozzle specification in the first place. Change the rig and the absolute rates move; the ranking of materials is more stable, but the numbers attached to it are not portable in the way a table of tensile strengths is.

Service conditions also arrive with company. In a hydro plant, cavitation comes with silt, dissolved oxygen and long submerged idle periods. On a marine propeller it comes with chloride. Erosion and corrosion together can remove material faster than either process alone, and a water jet is not built to capture that synergy.

Nor does MER describe a component's whole life. Standard practice distinguishes the maximum instantaneous rate from a terminal rate that may settle in later, and the headline metric here is the peak. The full open-access record, including the erosion curves and the property tables, is published through the paper's DOI at Tribology International, and a copy is archived in the University of Memphis faculty publications repository.

The case for caution

A turbine materials engineer would raise the surface question first. Cavitation resistance in these alloys depends on heat treatment, cold work, grain size and residual stress. Bronze from one foundry is not bronze from another, and a correlation built on single specimens says nothing about lot-to-lot scatter, which is the number a maintenance planner actually needs.

There's a wider point too. Cavitation damage is stochastic: bubble clouds are not uniform, and two specimens of the same alloy tested side by side will not lose identical mass. ASTM interlaboratory work has shown incubation time and maximum erosion rate scattering considerably more between labs than the tangent erosion rate does. Correlations drawn from a handful of specimens carry that noise with them.

None of which invalidates the finding. The direction of every correlation agrees with decades of field experience that tough, strong metals last longer under cavitating flow. What the paper adds is quantification across a deliberately wide material set, measured with one protocol, on one rig, by one group — a cleaner comparison than the literature usually offers.

Caution text overlay

Photo by Goh Rhy Yan on Unsplash

What changes for design and procurement

The practical takeaway is procedural. Where erosion is a design driver, specify a cavitating-jet test alongside the conventional mechanical properties, because the properties on a datasheet don't collapse into one another. Utilities already do something like this for coatings and weld overlays; the Bureau of Reclamation's long-running cavitation programme at Grand Coulee has spent more than a decade instrumenting Francis runners to map where damage accumulates and which operating ranges trigger it, and it treats material and operating envelope as a single problem. Read more on the Reclamation cavitation research page.

For alloy development, the paper's list of properties is a starting checklist:

  • Measure plastic indentation work, not just hardness, when screening candidates for a cavitating duty.
  • Include a high-strain-rate test, since the loading in service is nothing like a slow pull.
  • Treat toughness and ultimate strength as erosion-relevant, not just structural requirements.
  • Confirm the shortlist on a cavitating jet before committing to a production run of castings.

The additive manufacturing angle is where this could travel furthest. Keya's earlier work centred on laser powder bed fusion of nickel superalloys such as Inconel 625, where heat treatment is used to tune precipitate structure and hardness. Printed and coated surfaces create new microstructures at rates that conventional alloy handbooks have no data for. A screening protocol that combines indentation energy with jet erosion gives those new materials something to be measured against.

What would move this from a careful correlation study to a design tool is breadth. More alloys per family, several heats of each, and tests in water carrying silt and chloride would let someone build the lookup table that procurement wants. Cheaper, faster high-strain-rate testing would help too, since that data is currently the scarcest input in the analysis.

Until then, the useful sentence from this paper is a negative one: no single property decides how a metal performs under cavitation. Designers who act on that — asking for two or three measurements instead of one — will pick better alloys than the datasheet shortcut allows.

  • materials-science
  • tribology
  • hydropower
  • cavitation-erosion
  • tahmina-keya
Portrait of Jarrod Kanizay
About the author

Jarrod KanizayView author

Academic Jobs In House Author

Visionary leader transforming academic recruitment with 20+ years in higher education.

Discussion

Sort by:

Be the first to comment on this article!

You

You’ll be asked to sign in before your comment is posted.

Browse by Faculty

Browse by Subject

Frequently Asked Questions

💧What is cavitation erosion in simple terms?

Cavitation happens when a flowing liquid drops below its vapour pressure and forms vapour bubbles. When those bubbles reach a region of higher pressure they collapse violently, firing tiny jets of liquid at the metal surface beside them. Repeated thousands of times a second, those impacts pit, crack and eventually remove material. The result is cavitation erosion: surface damage caused by bubble collapse rather than by solid particles or chemical attack.

🔬What did Tahmina Keya's study actually test?

The team ran cavitation erosion tests using a cavitating liquid jet apparatus following the ASTM G134 practice on AA 6063 aluminium, pure copper, bronze, a copper-nickel alloy and 316L stainless steel. They then measured microhardness, plastic indentation work through depth-sensing indentation, and mechanical behaviour under quasi-static and high-strain-rate loading to extract toughness, ultimate strength and flow stress, and correlated those properties with the measured maximum erosion rate.

⚙️Why was AA 6063 aluminium 171 times worse than bronze?

AA 6063 aluminium had the highest maximum erosion rate of the materials tested, 171 times higher than bronze, the most erosion-resistant material in the set. The gap reflects the combination of properties the paper tracked: the aluminium is softer, absorbs less energy during indentation, and has lower toughness and ultimate strength than the bronze, so its surface deforms, cracks and breaks away under repeated bubble collapse far sooner.

📉What is the maximum erosion rate (MER)?

Maximum erosion rate is the steepest point on a cumulative erosion curve, the moment when material is being removed as fast as it ever will be during a test. Standard cavitation test practice characterises a material by several values taken from that curve, including the incubation period and the maximum instantaneous erosion rate. MER is a useful screening metric because it captures a material's worst-case behaviour rather than an average.

📏What is ASTM G134?

ASTM G134 is the standard practice for eroding solid materials with a cavitating liquid jet. Water is pumped through a specified nozzle into a chamber held at a controlled lower pressure, generating cavitation that collapses against a specimen mounted at a set stand-off distance. It is generally faster than the older vibratory method, ASTM G32, because the jet produces more aggressive cavitation, and it allows pressure and velocity effects to be evaluated.

🛠️Does hardness predict cavitation erosion resistance?

Only partly. The study found that maximum erosion rate falls as hardness rises, so hardness is a genuine indicator. But the authors state plainly that cavitation erosion does not correlate with a single property, and their toughness, ultimate strength and flow stress measurements tracked damage just as consistently. A materials specification that lists only hardness is therefore leaving out information that the paper shows to be relevant.

🧪What is plastic indentation work and why does it matter here?

Plastic indentation work is the energy a material absorbs while a hard indenter presses a permanent dent into its surface, measured with depth-sensing indentation equipment. It captures how much deformation a metal tolerates before it starts to fail, which is close to what a collapsing bubble does to a surface. In the study, materials with lower plastic indentation work eroded faster.

⚡Why did the researchers include high-strain-rate tests?

Because a collapsing cavitation bubble delivers its load in microseconds, not minutes. A conventional quasi-static tensile test loads a specimen slowly enough that the metal has time to accommodate the deformation. High-strain-rate testing deforms the material fast enough to resemble the impact conditions of cavitation. The paper reports that maximum erosion rate increases as high-strain-rate flow stress and ultimate strength decrease.

⚠️What are the main limitations of this study?

The material set is small: one aluminium alloy, three copper-based alloys and one stainless steel, tested as single specimens in one rig, at one jet intensity, with water as the working liquid. Published work on ASTM G134 has shown that erosion rates can vary by more than 600 percent with nozzle geometry, so absolute rates are rig-dependent. The experiments also did not capture erosion-corrosion synergy, which is common in real hydropower and marine service.

🏭Where does cavitation erosion cause problems in industry?

Common sites include hydroelectric turbine runners and guide vanes, pump impellers, ship propellers, valve trim, and the water-cooled passages of engine components. In hydropower, repairs are expensive and weld repair alters the blade profile, so material choice at the design stage affects maintenance costs and outage scheduling for years. Similar damage appears in diesel fuel injectors and in any high-velocity liquid system where local pressure drops.

🥉Does this mean bronze is always the best material choice?

No. Bronze performed best among the five materials in this specific test, but the paper's point is that erosion resistance follows a combination of hardness, indentation energy, strength and toughness rather than membership in a metal family. Cost, weight, corrosion behaviour, weldability and availability also drive selection. The useful conclusion is that erosion resistance should be measured, not inferred from one number on a certificate.

📄Where can I read the full paper?

The article, Influence of mechanical properties on cavitation-erosion via cavitating jet, by Keya, Shakil, Odeshi, Haghshenas, Choi and Hadadzadeh, appears in Tribology International volume 209 (2025), article 110754, and is available open access through its DOI. A record and full-text link are also archived in the University of Memphis faculty publications repository.